{"id":1813,"date":"2026-03-02T06:43:25","date_gmt":"2026-03-02T06:43:25","guid":{"rendered":"https:\/\/prigo.mx\/prigo-wip\/?page_id=1813"},"modified":"2026-03-02T06:43:26","modified_gmt":"2026-03-02T06:43:26","slug":"soldadura-del-acero-al-manganeso-12-14","status":"publish","type":"page","link":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/","title":{"rendered":"Soldadura del Acero al Manganeso 12-14%"},"content":{"rendered":"\n<div style=\"background-color: transparent; width: 100%; box-sizing: border-box; clear: both;\">\n\n    <div style=\"background-color: #000000; color: #ffffff; font-family: Arial, sans-serif; padding: 60px 20px; box-sizing: border-box; width: 100%; margin: 0;\">\n\n        <div style=\"max-width: 1000px; margin: 0 auto 50px auto; text-align: center; box-sizing: border-box;\">\n            <p style=\"color: #FF0000; text-transform: uppercase; letter-spacing: 2px; font-weight: bold; margin-bottom: 10px; font-size: 14px;\">Manual de Ingenier\u00eda<\/p>\n            <h1 style=\"color: #ffffff; text-transform: uppercase; font-size: 38px; margin-top: 0; margin-bottom: 15px; line-height: 1.2;\">Soldadura del Acero al Manganeso <span style=\"color: #FF0000;\">12-14%<\/span><\/h1>\n            <h2 style=\"color: #aaaaaa; font-size: 20px; font-weight: normal; margin-top: 0; margin-bottom: 40px;\">Recomendaciones Profesionales para el Acero Hadfield<\/h2>\n            \n            <img decoding=\"async\" src=\"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png\" alt=\"Proceso de soldadura industrial\" style=\"max-width: 100%; width: 400px; height: auto; border-radius: 8px; border-bottom: 4px solid #FF0000; margin-bottom: 30px; box-shadow: 0 10px 20px rgba(255,0,0,0.15);\">\n            \n            <p style=\"color: #cccccc; font-size: 18px; line-height: 1.6; max-width: 900px; margin: 0 auto;\">\n                El acero al manganeso es excepcional frente al desgaste, pero su soldadura requiere estrictos controles t\u00e9cnicos debido a su comportamiento metal\u00fargico. Este informe presenta las pr\u00e1cticas seguras para evitar la formaci\u00f3n de microestructuras fr\u00e1giles en la zona afectada por el calor (ZAC).\n            <\/p>\n        <\/div>\n\n        <div style=\"max-width: 1200px; margin: 0 auto 60px auto; box-sizing: border-box;\">\n            \n            <div style=\"display: flex; flex-wrap: wrap; gap: 30px; justify-content: center;\">\n                \n                <div style=\"flex: 1 1 calc(50% - 30px); min-width: 300px; background-color: #1a1a1a; padding: 40px; border-radius: 8px; border-top: 4px solid #FF0000; box-sizing: border-box;\">\n                    <h3 style=\"color: #ffffff; font-size: 22px; margin-top: 0; margin-bottom: 20px; text-transform: uppercase;\">1. Material de Aporte<\/h3>\n                    <p style=\"color: #cccccc; font-size: 15px; line-height: 1.6; margin-bottom: 15px;\">Para preservar la integridad austen\u00edtica, utilice consumibles con Mn &gt; 14% y carbono controlado:<\/p>\n                    <ul style=\"color: #aaaaaa; font-size: 15px; line-height: 1.7; padding-left: 20px; margin: 0;\">\n                        <li><strong>Electrodos sugeridos (SMAW):<\/strong> AWS A5.13 EFeMn-A o EFeMn-B.<\/li>\n                        <li><strong>Alambres (GMAW\/MIG):<\/strong> ERFeMn-A.<\/li>\n                        <li><strong>Prop\u00f3sito:<\/strong> Asegurar alta tenacidad y estructura completamente austen\u00edtica en el cord\u00f3n.<\/li>\n                    <\/ul>\n                <\/div>\n\n                <div style=\"flex: 1 1 calc(50% - 30px); min-width: 300px; background-color: #1a1a1a; padding: 40px; border-radius: 8px; border-top: 4px solid #FF0000; box-sizing: border-box;\">\n                    <h3 style=\"color: #ffffff; font-size: 22px; margin-top: 0; margin-bottom: 20px; text-transform: uppercase;\">2. Preparaci\u00f3n de Superficie<\/h3>\n                    <p style=\"color: #cccccc; font-size: 15px; line-height: 1.6; margin-bottom: 15px;\">Limpie completamente \u00f3xidos, grasas y material endurecido por trabajo (desbaste con esmeril):<\/p>\n                    <ul style=\"color: #aaaaaa; font-size: 15px; line-height: 1.7; padding-left: 20px; margin: 0;\">\n                        <li><strong>Espesor para preparaci\u00f3n:<\/strong> Desbastar de 3 a 5 mm.<\/li>\n                        <li><strong>\u00c1ngulo de bisel:<\/strong> Entre 60\u00b0 y 70\u00b0, dependiendo del espesor de la pieza.<\/li>\n                    <\/ul>\n                <\/div>\n\n                <div style=\"flex: 1 1 calc(50% - 30px); min-width: 300px; background-color: #1a1a1a; padding: 40px; border-radius: 8px; border-top: 4px solid #FF0000; box-sizing: border-box;\">\n                    <h3 style=\"color: #ffffff; font-size: 22px; margin-top: 0; margin-bottom: 20px; text-transform: uppercase;\">3. T\u00e9cnica y Par\u00e1metros<\/h3>\n                    <p style=\"color: #cccccc; font-size: 15px; line-height: 1.6; margin-bottom: 15px;\">Utilice cordones cortos y alternados para reducir la acumulaci\u00f3n de calor. Evite sobrepasar la zona de fusi\u00f3n m\u00e1s all\u00e1 de 3 mm.<\/p>\n                    <div style=\"background-color: #111111; padding: 15px; border-radius: 6px; border-left: 3px solid #FF0000;\">\n                        <p style=\"color: #ffffff; font-size: 14px; margin: 0 0 10px 0; text-transform: uppercase; font-weight: bold;\">Par\u00e1metros GMAW (MIG\/MAG):<\/p>\n                        <ul style=\"color: #aaaaaa; font-size: 14px; line-height: 1.6; padding-left: 20px; margin: 0;\">\n                            <li><strong>Voltaje:<\/strong> 24\u201330 V<\/li>\n                            <li><strong>Amperaje:<\/strong> 180\u2013280 A<\/li>\n                            <li><strong>Velocidad de avance:<\/strong> 20\u201330 cm\/min<\/li>\n                        <\/ul>\n                    <\/div>\n                <\/div>\n\n                <div style=\"flex: 1 1 calc(50% - 30px); min-width: 300px; background-color: #1a1a1a; padding: 40px; border-radius: 8px; border-top: 4px solid #FF0000; box-sizing: border-box;\">\n                    <h3 style=\"color: #ffffff; font-size: 22px; margin-top: 0; margin-bottom: 20px; text-transform: uppercase;\">4. Ensayos y Verificaci\u00f3n<\/h3>\n                    <p style=\"color: #cccccc; font-size: 15px; line-height: 1.6; margin-bottom: 15px;\">Para piezas sometidas a carga cr\u00edtica, se recomienda inspeccionar mediante:<\/p>\n                    <ul style=\"color: #aaaaaa; font-size: 15px; line-height: 1.7; padding-left: 20px; margin: 0;\">\n                        <li><strong>L\u00edquidos penetrantes:<\/strong> Detecci\u00f3n de fisuras superficiales.<\/li>\n                        <li><strong>Ultrasonido:<\/strong> Verificaci\u00f3n de integridad interna del cord\u00f3n.<\/li>\n                        <li><strong>Dureza y microestructura:<\/strong> Validaci\u00f3n final de la zona soldada.<\/li>\n                    <\/ul>\n                <\/div>\n\n            <\/div>\n        <\/div>\n\n        <div style=\"background-color: rgba(255,179,0,0.1); border: 2px solid #FFB300; padding: 40px; margin-bottom: 80px; box-sizing: border-box; max-width: 1000px; margin-left: auto; margin-right: auto; border-radius: 8px;\">\n            <h3 style=\"color: #FFB300; font-size: 24px; margin-top: 0; margin-bottom: 25px; text-transform: uppercase; text-align: center;\">\u26a0\ufe0f Control de Temperatura (Cr\u00edtico)<\/h3>\n            <p style=\"color: #cccccc; font-size: 16px; line-height: 1.6; margin-bottom: 20px; text-align: center;\">\n                El control t\u00e9rmico es fundamental para evitar la formaci\u00f3n de estructuras fr\u00e1giles y fisuras en el acero al manganeso.\n            <\/p>\n            \n            <div style=\"margin-bottom: 20px; text-align: center;\">\n                \n            <\/div>\n\n            <ul style=\"color: #ffffff; font-size: 16px; line-height: 1.8; padding-left: 20px; margin: 0;\">\n                <li style=\"margin-bottom: 10px;\"><strong>Precalentamiento:<\/strong> NO se recomienda, excepto en ambientes fr\u00edos (&lt; 10 \u00b0C), donde se debe precalentar a 100 \u2013 150 \u00b0C.<\/li>\n                <li style=\"margin-bottom: 10px;\"><strong>Temperatura interpasada:<\/strong> Mant\u00e9ngala siempre por debajo de los 260 \u00b0C.<\/li>\n                <li><strong style=\"color: #FF0000;\">Enfriamiento:<\/strong> Permita un enfriamiento r\u00e1pido al aire. <strong>NUNCA<\/strong> use m\u00e9todos de enfriamiento lento (como enterrar en arena o usar mantas de aislamiento t\u00e9rmico).<\/li>\n            <\/ul>\n        <\/div>\n\n        <div style=\"background-color: #FF0000; color: #ffffff; padding: 40px 20px; border-radius: 8px; text-align: center; max-width: 1200px; margin: 0 auto 60px auto; box-sizing: border-box;\">\n            <h2 style=\"margin-top: 0; margin-bottom: 15px; text-transform: uppercase; font-size: 28px;\">\u00bfRequiere Asistencia Experta?<\/h2>\n            <p style=\"margin-top: 0; margin-bottom: 25px; font-size: 16px; max-width: 800px; margin-left: auto; margin-right: auto;\">\n                En PRIGO somos expertos en el manejo y soldadura del acero al manganeso. Asegure el desempe\u00f1o de sus piezas bajo desgaste severo contactando a nuestro equipo de ingenieros.\n            <\/p>\n            <div style=\"display: flex; flex-wrap: wrap; gap: 30px; justify-content: center; font-size: 18px; font-weight: bold;\">\n                <span>\ud83d\udcde 442 228 38 64<\/span>\n                <span>\ud83d\udcf1 WA: 442 230 6743<\/span>\n                <span>\u2709\ufe0f ventasprigo1@outlook.com<\/span>\n            <\/div>\n        <\/div>\n\n        <div style=\"max-width: 900px; margin: 0 auto; background-color: #111111; padding: 40px; border-radius: 8px; border-left: 4px solid #333333; box-sizing: border-box;\">\n            <h3 style=\"color: #777777; text-transform: uppercase; font-size: 18px; margin-top: 0; margin-bottom: 25px; letter-spacing: 1px;\">Referencias Bibliogr\u00e1ficas<\/h3>\n            \n            <div style=\"margin-bottom: 15px; padding-left: 15px; border-left: 2px solid #FF0000;\">\n                <p style=\"color: #aaaaaa; font-size: 14px; margin: 0; line-height: 1.5;\">ASTM International. (2014). <em>ASTM A128\/A128M-14: Standard Specification for Steel Castings, Austenitic Manganese<\/em>. <a href=\"https:\/\/standards.iteh.ai\/catalog\/standards\/astm\/3f5702cf-ad07-4d9e-a32b-c3454869fe60\/astm-a128-a128m-19\" target=\"_blank\" style=\"color: #FF0000; text-decoration: none;\">[Ver ref.]<\/a><\/p>\n            <\/div>\n            <div style=\"margin-bottom: 15px; padding-left: 15px; border-left: 2px solid #FF0000;\">\n                <p style=\"color: #aaaaaa; font-size: 14px; margin: 0; line-height: 1.5;\">American Welding Society (AWS). <em>Welding Certifications, Courses &#038; Resources for Welding Professionals<\/em>. <a href=\"https:\/\/www.aws.org\/\" target=\"_blank\" style=\"color: #FF0000; text-decoration: none;\">[Ver ref.]<\/a><\/p>\n            <\/div>\n            <div style=\"margin-bottom: 15px; padding-left: 15px; border-left: 2px solid #FF0000;\">\n                <p style=\"color: #aaaaaa; font-size: 14px; margin: 0; line-height: 1.5;\">CompraCo. (2024). <em>How to weld high manganese steel?<\/em> <a href=\"https:\/\/compraco.com.br\/en\/blogs\/industria\/como-soldar-aco-com-alto-teor-de-manganes\" target=\"_blank\" style=\"color: #FF0000; text-decoration: none;\">[Ver ref.]<\/a><\/p>\n            <\/div>\n            <div style=\"margin-bottom: 15px; padding-left: 15px; border-left: 2px solid #FF0000;\">\n                <p style=\"color: #aaaaaa; font-size: 14px; margin: 0; line-height: 1.5;\">ASM International. (1990). <em>ASM Handbook, Volume 1: Properties and Selection<\/em>. <a href=\"https:\/\/www.amazon.com\/ASM-Handbook-Properties-Selection-High-Performance\/dp\/0871703777\" target=\"_blank\" style=\"color: #FF0000; text-decoration: none;\">[Ver ref.]<\/a><\/p>\n            <\/div>\n            <div style=\"margin-bottom: 0; padding-left: 15px; border-left: 2px solid #FF0000;\">\n                <p style=\"color: #aaaaaa; font-size: 14px; margin: 0; line-height: 1.5;\">Zellagui, R., et al. (2019). <em>Effect of Element Addition, Microstructure Characteristics, Mechanical Properties, Machining and Welding Processes of the Hadfield Austenitic Manganese Steel<\/em>. <a href=\"https:\/\/doaj.org\/article\/8f3f1a2547f34005be19b910c5fa364a\" target=\"_blank\" style=\"color: #FF0000; text-decoration: none;\">[Ver ref.]<\/a><\/p>\n            <\/div>\n        <\/div>\n\n    <\/div>\n<\/div>\n","protected":false},"excerpt":{"rendered":"<p>Manual de Ingenier\u00eda Soldadura del Acero al Manganeso 12-14% Recomendaciones Profesionales para el Acero Hadfield El acero al manganeso es excepcional frente al desgaste, pero su soldadura requiere estrictos controles t\u00e9cnicos debido a su comportamiento metal\u00fargico. Este informe presenta las pr\u00e1cticas seguras para evitar la formaci\u00f3n de microestructuras fr\u00e1giles en la zona afectada por el [&hellip;]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"full-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"_joinchat":[],"footnotes":""},"class_list":["post-1813","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v27.3 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.\" \/>\n<meta property=\"og:description\" content=\"Manual de Ingenier\u00eda Soldadura del Acero al Manganeso 12-14% Recomendaciones Profesionales para el Acero Hadfield El acero al manganeso es excepcional frente al desgaste, pero su soldadura requiere estrictos controles t\u00e9cnicos debido a su comportamiento metal\u00fargico. Este informe presenta las pr\u00e1cticas seguras para evitar la formaci\u00f3n de microestructuras fr\u00e1giles en la zona afectada por el [&hellip;]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/\" \/>\n<meta property=\"og:site_name\" content=\"PRIGO ACEROS ESPECIALES S.A. de C.V.\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/share\/1Ag2aeUQAx\/\" \/>\n<meta property=\"article:modified_time\" content=\"2026-03-02T06:43:26+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"3 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/\",\"url\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/\",\"name\":\"Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/prigo.mx\\\/wp-content\\\/uploads\\\/2025\\\/05\\\/PUBLIC-8-PG-300x251.png\",\"datePublished\":\"2026-03-02T06:43:25+00:00\",\"dateModified\":\"2026-03-02T06:43:26+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/#primaryimage\",\"url\":\"https:\\\/\\\/prigo.mx\\\/wp-content\\\/uploads\\\/2025\\\/05\\\/PUBLIC-8-PG-300x251.png\",\"contentUrl\":\"https:\\\/\\\/prigo.mx\\\/wp-content\\\/uploads\\\/2025\\\/05\\\/PUBLIC-8-PG-300x251.png\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/soldadura-del-acero-al-manganeso-12-14\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Portada\",\"item\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Soldadura del Acero al Manganeso 12-14%\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#website\",\"url\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/\",\"name\":\"prigo.mx\",\"description\":\"Soluciones f\u00e1ciles para aplicaciones dif\u00edciles\",\"publisher\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#organization\",\"name\":\"Prigo Aceros Especiales S.A. de C.V.\",\"url\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/prigo.mx\\\/wp-content\\\/uploads\\\/2023\\\/02\\\/cropped-cropped-LOGO-PRIGO2-1-1-1.png\",\"contentUrl\":\"https:\\\/\\\/prigo.mx\\\/wp-content\\\/uploads\\\/2023\\\/02\\\/cropped-cropped-LOGO-PRIGO2-1-1-1.png\",\"width\":1794,\"height\":1795,\"caption\":\"Prigo Aceros Especiales S.A. de C.V.\"},\"image\":{\"@id\":\"https:\\\/\\\/prigo.mx\\\/prigo-wip\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/share\\\/1Ag2aeUQAx\\\/\",\"https:\\\/\\\/www.instagram.com\\\/prigoacerosespeciales?igsh=YnFtaGJ2cjRyNjN4\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/prigo-aceros-de-importacin\\\/?viewAsMember=true\"]}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/","og_locale":"es_ES","og_type":"article","og_title":"Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.","og_description":"Manual de Ingenier\u00eda Soldadura del Acero al Manganeso 12-14% Recomendaciones Profesionales para el Acero Hadfield El acero al manganeso es excepcional frente al desgaste, pero su soldadura requiere estrictos controles t\u00e9cnicos debido a su comportamiento metal\u00fargico. Este informe presenta las pr\u00e1cticas seguras para evitar la formaci\u00f3n de microestructuras fr\u00e1giles en la zona afectada por el [&hellip;]","og_url":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/","og_site_name":"PRIGO ACEROS ESPECIALES S.A. de C.V.","article_publisher":"https:\/\/www.facebook.com\/share\/1Ag2aeUQAx\/","article_modified_time":"2026-03-02T06:43:26+00:00","og_image":[{"url":"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"3 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/","url":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/","name":"Soldadura del Acero al Manganeso 12-14% - PRIGO ACEROS ESPECIALES S.A. de C.V.","isPartOf":{"@id":"https:\/\/prigo.mx\/prigo-wip\/#website"},"primaryImageOfPage":{"@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/#primaryimage"},"image":{"@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/#primaryimage"},"thumbnailUrl":"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png","datePublished":"2026-03-02T06:43:25+00:00","dateModified":"2026-03-02T06:43:26+00:00","breadcrumb":{"@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/"]}]},{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/#primaryimage","url":"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png","contentUrl":"https:\/\/prigo.mx\/wp-content\/uploads\/2025\/05\/PUBLIC-8-PG-300x251.png"},{"@type":"BreadcrumbList","@id":"https:\/\/prigo.mx\/prigo-wip\/soldadura-del-acero-al-manganeso-12-14\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Portada","item":"https:\/\/prigo.mx\/prigo-wip\/"},{"@type":"ListItem","position":2,"name":"Soldadura del Acero al Manganeso 12-14%"}]},{"@type":"WebSite","@id":"https:\/\/prigo.mx\/prigo-wip\/#website","url":"https:\/\/prigo.mx\/prigo-wip\/","name":"prigo.mx","description":"Soluciones f\u00e1ciles para aplicaciones dif\u00edciles","publisher":{"@id":"https:\/\/prigo.mx\/prigo-wip\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/prigo.mx\/prigo-wip\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/prigo.mx\/prigo-wip\/#organization","name":"Prigo Aceros Especiales S.A. de C.V.","url":"https:\/\/prigo.mx\/prigo-wip\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/prigo.mx\/prigo-wip\/#\/schema\/logo\/image\/","url":"https:\/\/prigo.mx\/wp-content\/uploads\/2023\/02\/cropped-cropped-LOGO-PRIGO2-1-1-1.png","contentUrl":"https:\/\/prigo.mx\/wp-content\/uploads\/2023\/02\/cropped-cropped-LOGO-PRIGO2-1-1-1.png","width":1794,"height":1795,"caption":"Prigo Aceros Especiales S.A. de C.V."},"image":{"@id":"https:\/\/prigo.mx\/prigo-wip\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/share\/1Ag2aeUQAx\/","https:\/\/www.instagram.com\/prigoacerosespeciales?igsh=YnFtaGJ2cjRyNjN4","https:\/\/www.linkedin.com\/company\/prigo-aceros-de-importacin\/?viewAsMember=true"]}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false},"uagb_author_info":{"display_name":"Prigo","author_link":"https:\/\/prigo.mx\/prigo-wip\/author\/prigo\/"},"uagb_comment_info":0,"uagb_excerpt":"Manual de Ingenier\u00eda Soldadura del Acero al Manganeso 12-14% Recomendaciones Profesionales para el Acero Hadfield El acero al manganeso es excepcional frente al desgaste, pero su soldadura requiere estrictos controles t\u00e9cnicos debido a su comportamiento metal\u00fargico. Este informe presenta las pr\u00e1cticas seguras para evitar la formaci\u00f3n de microestructuras fr\u00e1giles en la zona afectada por el&hellip;","_links":{"self":[{"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/pages\/1813","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/comments?post=1813"}],"version-history":[{"count":1,"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/pages\/1813\/revisions"}],"predecessor-version":[{"id":1814,"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/pages\/1813\/revisions\/1814"}],"wp:attachment":[{"href":"https:\/\/prigo.mx\/prigo-wip\/wp-json\/wp\/v2\/media?parent=1813"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}